压铸缺陷英文 Last updated at 10:00 am on 25th December 2020 磕碰:knockedwounded
划伤: scratch
变形:bending warping
拉伤:drags
卧式钻床>广告检测龟裂:turtle cracks,network cracks
夹杂:inclusions
锈蚀,发霉:rust,corrosion
裂纹:cracks
气泡:blisters
气孔:gas porosity
网架滑动支座
油污:stained casting
夹层:laminations
成形不良:non-fills
零件外观不允许有明显压铸缺陷如冷隔、发黑拉伤、起皮、水纹、粘料、切伤、滑块凸起
cold shut,black surface,drag mark,stripping,wave,sticky material,trimming wound and raised slider are not allowed on parts
• A . 尺寸,形状缺陷
•铸造缺陷 casting defects
•尺寸超差 improper shrinkage allowance
•尺寸不合格 wrong size
•模样错误 excess rapping of pattern, deformed pattern,•壁厚不均 different thickness
•铸型下垂 mold sag
•错型 mold shift, shift, miss-match, cross-joint •舂移 ram off, ram away
•塌型 mold drop, drop off, drop out, drop sticker 上型下沉,沉芯 sag( 上型和型芯下垂导致壁厚减小)
•飞翅 fins, joint flash
•翘曲 warp age, buckling, warping, camber
•铸件变形 warped casting
•挤箱 push up, cramp-off
•型裂 broken mold, cracked
•掉砂 crush of mold, crush
接线排•变形 deformation, casting distortion, warped casting • B. 缩孔(由凝固收缩引起 ) •缩孔 shrinkage, shrinkaged cavity
•内部缩孔 internal shrinkage, dispersed shrinkage, blind shrinkage
•敞露缩孔 open shrinkage, external shrinkages, sink marks, depression •缩松 porosity, shrinkage porosity, leakers, micro shrinkage, disperded shrinkage
滑水鞋
•缩陷 sink marks, draw, suck-in
•芯面缩孔 core shrinkage
•内角缩孔 corner shrinkage, fillet shrinkage
•出汗孔 extruded bead, exudation
•线状缩孔 fissure like shrinkage
• C. 气体缺陷(由气体引起的孔)
•气孔 blowholes, gas hole, blow
•针孔 pinholes
•裂纹状缺陷,线状缺陷 fissure defects
• D. 裂纹
•裂纹 crack
•缩裂 shrinkage crack
•季裂 season cracking, season crack
•应力热裂 hot cracking, hot tearing, hot tear •淬火裂纹 quench crack, quenching crack
•应力冷裂 cold cracking, breakage, cold tearing, cold tear •龟裂 crack
•激冷层裂纹,白裂 chill crack
• E. 夹杂物
•夹渣 slag inclusion, slag blowholes
•砂眼 sand inclusion, raised sand, sand hole
•其他夹杂物 the other inclusion
太阳能取暖房
•胀砂 push up, cramp-off, sand hole
•掉砂 crush, crush of mold